Lincoln Electric C2.410 Welding System User Manual


 
-14-
Flat Fillet Welds
Also see Low Hydrogen Procedures.
For X-ray quality:
1. Use low hydrogen procedures, pages 24-34.
(or)
2. Weld 3/16” to 5/16” fillets with E6027 electrodes at the E7024
procedures. Weld 3/8” and larger fillets with 1/4” E6027 at
about 400 amps. Travel speed will be slower.
T
L
Plate Size – T 14 ga 12 ga 10 ga 3/16" 3/16" 1/4" 1/4"
No. of Passes 1 1 1 1 1 1 1
Leg Size – L (in.) 5/32 5/32 3/16 3/16
Electrode/AWS Class Jetweld 1/E7024-1
Diameter (in.) 3/32 1/8 1/8 1/8 5/32 5/32 3/16
Current (Amps) 95 150 160 180 210 230 270
Polarity AC AC AC AC AC AC AC
Arc Speed In./Min.
(1)
15 17-1/2 17-1/2 17 16-1/2 17 14-1/2
Ft. of Weld/Hr.
(2)
75 88 88 85 83 85 72
Lbs. of Elec./Ft. of .049 .076 .082 .117 .162 .20 .29
Weld
(1) First pass only. On later passes adjust arc speed to obtain proper
bead size.
(2) Total for all passes. 100% operating factor.