Seiko Group OFL-12 SERIES Sander User Manual


 
4 - 13
4.6 POLISHING CONDITION CHECK
Check the condition of the ferrule tips after polishing. If there was a deep scratch
caused in the fiber during the adhesive removal step, satisfactory polishing cannot
be obtained. In this case, repolish.
NOTE
When repolishing ferrules that have an unsatisfactory polished condition,
polish from the grinding step to the finishing step to obtain consistent
polished quality.
(1) Speckles (2) Slight Scratch
Speckles
Slight scratch
Repolish, doin
g
the polishin
g
and
finishing steps.
Occurs near the end of the life of
the polishing film.
Occurs when the ferrule
mountin
g
in the holding jig is poor.
Repolish, doin
g
the polishin
g
and
finishing steps.
Occurs when there is insufficient
cleanin
g
between polishin
g
steps.
Occurs when you rub the tips of
the ferrules a
g
ainst the polishin
g
film when mountin
g
the holdin
g
ji
g
to and removin
g
it from the
polishing unit.